Chemical Composition
C % | Si % | Mn % | P % | S % | Cr % | Mo % | N % | Ni % |
max 0,05 | max 0,70 | max 1,50 | max 0,040 | max 0,015 | 12,00 - 14,00 | 0,30 - 0,70 | max 0,020 | 3,50 - 4,50 |
Mechanical Properties
DIN EN 10088-3 (12/2014) Nichtrostende Stähle. Halbzeug, Stäbe, Walzdraht, gezogener Draht, Profile und Blankstahlerzeugnisse aus korrosionsbeständigen Stählen für allgemeine Verwendung. | |||
Stäbe | |||
geglüht | Zugfestigkeit (Rm) | Härte [HBW] | bei Temperatur |
<= 1.100 N/mm² | <= 320 HBW | ~ 20 ° C |
vergütet | 0,2% Dehngrenze (Rp0,2) / bei Temperatur | Zugfestigkeit (Rm) | Bruchdehnung (A 5,65) | Kerbschlagarbeit KV2 (ISO-V/Charpy-V) | Probenlage |
160 - 250 mm | >= 800 N/mm² / ~ 20 ° C | 900 - 1.100 N/mm² | >= 12 % | >= 50 Joule | quer |
160 - 250 mm | >= 620 N/mm² / ~ 20 ° C | 780 - 980 N/mm² | >= 12 % | >= 70 Joule | quer |
160 - 250 mm | >= 520 N/mm² / ~ 20 ° C | 700 - 850 N/mm² | >= 10 % | >= 70 Joule | quer |
<= 160 mm | >= 800 N/mm² / ~ 20 ° C | 900 - 1.100 N/mm² | >= 15 % | >= 40 Joule | längs |
<= 160 mm | >= 620 N/mm² / ~ 20 ° C | 780 - 980 N/mm² | >= 15 % | >= 50 Joule | längs |
<= 160 mm | >= 520 N/mm² / ~ 20 ° C | 700 - 850 N/mm² | >= 12 % | >= 50 Joule | längs |
>= 515 N/mm² / ~ 350 ° C | |||||
>= 450 N/mm² / ~ 350 ° C | |||||
>= 620 N/mm² / ~ 300 ° C | |||||
>= 530 N/mm² / ~ 300 ° C | |||||
>= 460 N/mm² / ~ 300 ° C | |||||
>= 640 N/mm² / ~ 250 ° C | |||||
>= 545 N/mm² / ~ 250 ° C | |||||
>= 470 N/mm² / ~ 250 ° C | |||||
>= 665 N/mm² / ~ 200 ° C | |||||
>= 560 N/mm² / ~ 200 ° C | |||||
>= 480 N/mm² / ~ 200 ° C | |||||
>= 690 N/mm² / ~ 150 ° C | |||||
>= 575 N/mm² / ~ 150 ° C | |||||
>= 490 N/mm² / ~ 150 ° C | |||||
>= 720 N/mm² / ~ 100 ° C | |||||
>= 590 N/mm² / ~ 100 ° C | |||||
>= 500 N/mm² / ~ 100 ° C |
Halbzeug | |||
geglüht | Zugfestigkeit (Rm) | Härte [HBW] | bei Temperatur |
<= 1.100 N/mm² | <= 320 HBW | ~ 20 ° C |
vergütet | 0,2% Dehngrenze (Rp0,2) / bei Temperatur | Zugfestigkeit (Rm) | Bruchdehnung (A 5,65) | Kerbschlagarbeit KV2 (ISO-V/Charpy-V) | Probenlage |
160 - 250 mm | >= 800 N/mm² / ~ 20 ° C | 900 - 1.100 N/mm² | >= 12 % | >= 50 Joule | quer |
160 - 250 mm | >= 620 N/mm² / ~ 20 ° C | 780 - 980 N/mm² | >= 12 % | >= 70 Joule | quer |
160 - 250 mm | >= 520 N/mm² / ~ 20 ° C | 700 - 850 N/mm² | >= 10 % | >= 70 Joule | quer |
<= 160 mm | >= 800 N/mm² / ~ 20 ° C | 900 - 1.100 N/mm² | >= 15 % | >= 40 Joule | längs |
<= 160 mm | >= 620 N/mm² / ~ 20 ° C | 780 - 980 N/mm² | >= 15 % | >= 50 Joule | längs |
<= 160 mm | >= 520 N/mm² / ~ 20 ° C | 700 - 850 N/mm² | >= 12 % | >= 50 Joule | längs |
>= 515 N/mm² / ~ 350 ° C | |||||
>= 450 N/mm² / ~ 350 ° C | |||||
>= 620 N/mm² / ~ 300 ° C | |||||
>= 530 N/mm² / ~ 300 ° C | |||||
>= 460 N/mm² / ~ 300 ° C | |||||
>= 640 N/mm² / ~ 250 ° C | |||||
>= 545 N/mm² / ~ 250 ° C | |||||
>= 470 N/mm² / ~ 250 ° C | |||||
>= 665 N/mm² / ~ 200 ° C | |||||
>= 560 N/mm² / ~ 200 ° C | |||||
>= 480 N/mm² / ~ 200 ° C | |||||
>= 690 N/mm² / ~ 150 ° C | |||||
>= 575 N/mm² / ~ 150 ° C | |||||
>= 490 N/mm² / ~ 150 ° C | |||||
>= 720 N/mm² / ~ 100 ° C | |||||
>= 590 N/mm² / ~ 100 ° C | |||||
>= 500 N/mm² / ~ 100 ° C |
Walzdraaht | ||
geglüht | Zugfestigkeit (Rm) | bei Temperatur |
<= 1.100 N/mm² | ~ 20 ° C |
vergütet | Zugfestigkeit (Rm) | bei Temperatur |
160 - 250 mm | 900 - 1.100 N/mm² | ~ 20 ° C |
160 - 250 mm | 780 - 980 N/mm² | ~ 20 ° C |
160 - 250 mm | 700 - 850 N/mm² | ~ 20 ° C |
<= 160 mm | 900 - 1.100 N/mm² | ~ 20 ° C |
<= 160 mm | 780 - 980 N/mm² | ~ 20 ° C |
<= 160 mm | 700 - 850 N/mm² | ~ 20 ° C |
Gezogener Draht | |||
geglüht | Zugfestigkeit (Rm) | Härte [HBW] | bei Temperatur |
<= 1.100 N/mm² | <= 320 HBW | ~ 20 ° C |
vergütet | 0,2% Dehngrenze (Rp0,2) / bei Temperatur | Zugfestigkeit (Rm) | Bruchdehnung (A 5,65) | Kerbschlagarbeit KV2 (ISO-V/Charpy-V) | Probenlage |
160 - 250 mm | >= 800 N/mm² / ~ 20 ° C | 900 - 1.100 N/mm² | >= 12 % | >= 50 Joule | quer |
160 - 250 mm | >= 620 N/mm² / ~ 20 ° C | 780 - 980 N/mm² | >= 12 % | >= 70 Joule | quer |
160 - 250 mm | >= 520 N/mm² / ~ 20 ° C | 700 - 850 N/mm² | >= 10 % | >= 70 Joule | quer |
<= 160 mm | >= 800 N/mm² / ~ 20 ° C | 900 - 1.100 N/mm² | >= 15 % | >= 40 Joule | längs |
<= 160 mm | >= 620 N/mm² / ~ 20 ° C | 780 - 980 N/mm² | >= 15 % | >= 50 Joule | längs |
<= 160 mm | >= 520 N/mm² / ~ 20 ° C | 700 - 850 N/mm² | >= 12 % | >= 50 Joule | längs |
>= 515 N/mm² / ~ 350 ° C | |||||
>= 450 N/mm² / ~ 350 ° C | |||||
>= 620 N/mm² / ~ 300 ° C | |||||
>= 530 N/mm² / ~ 300 ° C | |||||
>= 460 N/mm² / ~ 300 ° C | |||||
>= 640 N/mm² / ~ 250 ° C | |||||
>= 545 N/mm² / ~ 250 ° C | |||||
>= 470 N/mm² / ~ 250 ° C | |||||
>= 665 N/mm² / ~ 200 ° C | |||||
>= 560 N/mm² / ~ 200 ° C | |||||
>= 480 N/mm² / ~ 200 ° C | |||||
>= 690 N/mm² / ~ 150 ° C | |||||
>= 575 N/mm² / ~ 150 ° C | |||||
>= 490 N/mm² / ~ 150 ° C | |||||
>= 720 N/mm² / ~ 100 ° C | |||||
>= 590 N/mm² / ~ 100 ° C | |||||
>= 500 N/mm² / ~ 100 ° C |
Profile | |||
geglüht | Zugfestigkeit (Rm) | Härte [HBW] | bei Temperatur |
<= 1.100 N/mm² | <= 320 HBW | ~ 20 ° C |
vergütet | 0,2% Dehngrenze (Rp0,2) / bei Temperatur | Zugfestigkeit (Rm) | Bruchdehnung (A 5,65) | Kerbschlagarbeit KV2 (ISO-V/Charpy-V) | Probenlage |
160 - 250 mm | >= 800 N/mm² / ~ 20 ° C | 900 - 1.100 N/mm² | >= 12 % | >= 50 Joule | quer |
160 - 250 mm | >= 620 N/mm² / ~ 20 ° C | 780 - 980 N/mm² | >= 12 % | >= 70 Joule | quer |
160 - 250 mm | >= 520 N/mm² / ~ 20 ° C | 700 - 850 N/mm² | >= 10 % | >= 70 Joule | quer |
<= 160 mm | >= 800 N/mm² / ~ 20 ° C | 900 - 1.100 N/mm² | >= 15 % | >= 40 Joule | längs |
<= 160 mm | >= 620 N/mm² / ~ 20 ° C | 780 - 980 N/mm² | >= 15 % | >= 50 Joule | längs |
<= 160 mm | >= 520 N/mm² / ~ 20 ° C | 700 - 850 N/mm² | >= 12 % | >= 50 Joule | längs |
>= 515 N/mm² / ~ 350 ° C | |||||
>= 450 N/mm² / ~ 350 ° C | |||||
>= 620 N/mm² / ~ 300 ° C | |||||
>= 530 N/mm² / ~ 300 ° C | |||||
>= 460 N/mm² / ~ 300 ° C | |||||
>= 640 N/mm² / ~ 250 ° C | |||||
>= 545 N/mm² / ~ 250 ° C | |||||
>= 470 N/mm² / ~ 250 ° C | |||||
>= 665 N/mm² / ~ 200 ° C | |||||
>= 560 N/mm² / ~ 200 ° C | |||||
>= 480 N/mm² / ~ 200 ° C | |||||
>= 690 N/mm² / ~ 150 ° C | |||||
>= 575 N/mm² / ~ 150 ° C | |||||
>= 490 N/mm² / ~ 150 ° C | |||||
>= 720 N/mm² / ~ 100 ° C | |||||
>= 590 N/mm² / ~ 100 ° C | |||||
>= 500 N/mm² / ~ 100 ° C |