Material 1.3207
Acero de alta velocidad
1.3207 is a high speed steel with good edge-holding properties, a high temperature hardness as well as a good hardiness. IT is being used for cutting tools as well as milling tools.
Do you have any questions about the material or would you like to order? Complete our inquiry form, it`s free of charge and without obligation. We will get in touch with you in order to provide you with more information.
Standards
HDIN / EN | US-Standard | AFNOR | UNI | JIS | request |
---|---|---|---|---|---|
HS10-4-3-10 S10-4-3-10 | HS10-4-3-10 | SKH57 | request |
Material Category: Acero de alta velocidad
Chemical Composition
C % | Si % | Mn % | P % | S % | Co % | Cr % | Mo % | V % | W % |
1,20 - 1,35 | max 0,45 | max 0,40 | max 0,030 | max 0,030 | 9,50 - 10,50 | 3,80 - 4,50 | 3,20 - 3,90 | 3,00 - 3,50 | 9,00 - 10,00 |
Mechanical Properties
geglüht | <= 302 HBW |
gehärtet | ~ 66 HRC |
angelassen bei ~ 50 ° C | ~ 66 HRC |
angelassen bei ~ 300 ° C | ~ 61 HRC |
angelassen bei ~ 350 ° C | ~ 61,2 HRC |
angelassen bei ~ 400 ° C | ~ 62 HRC |
angelassen bei ~ 450 ° C | ~ 64 HRC |
angelassen bei ~ 500 ° C | ~ 66 HRC |
angelassen bei ~ 550 ° C | ~ 67 HRC |
angelassen bei ~ 600 ° C | ~ 65 HRC |
angelassen bei ~ 650 ° C | ~ 62 HRC |
angelassen bei ~ 700 ° C | ~ 55 HRC |
gehärtet und angelassen | >= 66 HRC |
geglüht und kaltgewalzt | <= 372 HBW |
geglüht und kaltgezogen | <= 352 HBW |
Material request