Material 1.7219
Tough at subzero steel
The material 1.7219 is a low-temperature structural steel. 1.7219 has a tensile strength of 590 - 740 N/mm² at room temperature and a yield strength of at least 440 N/mm². Screws and connecting elements are often made from 1.7219. This material is used up to approx. - 65 C°.
Do you have any questions about the material or would you like to order? Complete our inquiry form, it`s free of charge and without obligation. We will get in touch with you in order to provide you with more information.
Standards
Material Category: Tough at subzero steel
Chemical Composition
C % | Si % | Mn % | P % | S % | Cr % | Mo % |
0,22 - 0,29 | max 0,35 | 0,50 - 0,80 | max 0,025 | max 0,020 | 0,90 - 1,20 | 0,15 - 0,30 |
Product Specifications
DIN EN 10216-4 (03/2014)
Mechanical Properties
Streckgrenze (Re) | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Kerbschlagarbeit KV (ISO-V/Charpy-V) | bei Temperatur |
>= 590 N/mm² | >= 780 N/mm² | >= 14 % | >= 21Joule | ~ -120 ° C |
>= 540 N/mm² | >= 720 N/mm² | >= 15 % | >= 34 Joule | ~ -80 ° C |
>= 490 N/mm² | >= 670 N/mm² | >= 16 % | >= 48 Joule | ~ -50 ° C |
>= 470 N/mm² | >= 640 N/mm² | >= 17 % | >= 62 Joule | ~ -20 ° C |
vergütet | Streckgrenze (Re) | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Einschnürung (Z) | Kerbschlagarbeit KV (ISO-V/Charpy-V) |
<= 50 mm | >= 440 N/mm² | 590 - 740 N/mm² | >= 18 % | >= 60 % | >= 82 Joule |
Material request