Material 1.4948
High-temperature resisting steel and alloy
1.448 is a austenitic stainless steel. The material 1.4948 has very good strength values at elevated temperatures. These properties made of material with its high carbon content. It is also resistant to most acids oxidize. Often this material is used in power plants.
Do you have any questions about the material or would you like to order? Complete our inquiry form, it`s free of charge and without obligation. We will get in touch with you in order to provide you with more information.
Standards
HDIN / EN | US-Standard | AFNOR | UNI | JIS | request |
---|---|---|---|---|---|
X6CrNi18-10 | AISI 304H UNS S30409 UNS S304080 | SUS302 SUS304HFB SUS304HFB SUS304HTB SUS304HTP | request |
Material Category: High-temperature resisting steel and alloy
Chemical Composition
C % | Si % | Mn % | P % | S % | Cr % | N % | Ni % |
0,04 - 0,08 | max 1,00 | max 2,00 | max 0,035 | max 0,015 | 17,00 - 19,00 | max 0,100 | 8,00 - 11,00 |
Mechanical Properties
vergütet | ||||||||
0,2% Dehngrenze (Rp0,2) | Zugfestigkeit (Rm) | Bruchdehnung (A 5,65) | Kerbschlagarbeit (DVM) | Kerbschlagarbeit KV (ISO-V/Charpy-V) | Zeitstandfestigkeit 10.000 h | Zeitstandfestigkeit 100.000 h | Warmfestigkeit | bei Temperatur |
~ 650 °C | ||||||||
>= 185 N/mm² | 500 - 700 N/mm² | >= 40 % | >= 85 Joule | >= 90 Joule | ~ 20 °C | |||
>= 157 N/mm² | ~ 200 °C | |||||||
>= 127 N/mm² | ~ 300 °C | |||||||
>= 108 N/mm² | ~ 400 °C | |||||||
>= 98 N/mm² | ~ 500 °C | |||||||
>= 88 N/mm² | ~ 191 N/mm² | ~ 140 N/mm² | ~ 550 °C | |||||
>= 83 N/mm² | ~ 132 N/mm² | ~ 89 N/mm² | ~ 600 °C | |||||
>= 78 N/mm² | ~ 87 N/mm² | ~ 52 N/mm² | ~ 650 °C | |||||
>= 69 N/mm² | ~ 55 N/mm² | ~ 28 N/mm² | ~ 700 °C | |||||
~ 34 N/mm² | ~ 15 N/mm² | ~ 750 °C |