Material 1.4876
Heat-resisting steel
The material 1.4876 is a austenitic heat resistant steel. 1.4876 has good resistance in oxidizing and reducing atmospheres. This material is commonly used in furnace and appartus engineering. 1.4876 is also known as Alloy 800.
Do you have any questions about the material or would you like to order? Complete our inquiry form, it`s free of charge and without obligation. We will get in touch with you in order to provide you with more information.
Standards
HDIN / EN | US-Standard | AFNOR | UNI | JIS | request |
---|---|---|---|---|---|
X10NiCrAlTi32-21 X10NiCrAlTi32-20 | UNS N08800 UNS N08810 UNS N08332 UNS N08811 | NCF800 NCF800HTF NCF800TB NCF800TF NCF800TP | request |
Material Category: Heat-resisting steel
Chemical Composition
C % | Si % | Mn % | P % | S % | Al % | Cr % | Ni % | Ti % |
max 0,12 | max 1,00 | max 2,00 | max 0,030 | max 0,015 | 0,1500 - 0,6000 | 19,00 - 23,00 | 30,00 - 34,00 | 0,15 - 0,60 |
Mechanical Properties
DIN EN 10095 (12/2018 (05/1999)) Hitzebeständige Stähle und Nickellegierungen. | |||||
Zeitdehngrenze 1.000 h (Rp 1,0) | Zeitdehngrenze 10.000 h (Rp 1,0) | Zeitstandfestigkeit 1.000 h | Zeitstandfestigkeit 10.000 | Zeitstandfestigkeit 100.000 h | bei Temperatur |
~ 130 N/mm² | ~ 90 N/mm² | ~ 200 N/mm² | ~ 152 N/mm² | ~ 114 N/mm² | ~ 600 ° C |
~ 70 N/mm² | ~ 40 N/mm² | ~ 68 N/mm² | ~ 68 N/mm² | ~ 48 N/mm² | ~ 700 ° C |
~ 30 N/mm² | ~ 15 N/mm² | ~ 30 N/mm² | ~ 30 N/mm² | ~ 21 N/mm² | ~ 800 ° C |
~ 13 N/mm² | ~ 5 N/mm² | ~ 10 N/mm² | ~ 10 N/mm² | ~ 8 N/mm² | ~ 900 ° C |
Flacherzeugnisse | |||
lösungsgeglüht | Bruchdehnung (A5, 65) | Probenlage | bei Temperatur |
0,5 - 3 mm | >= 28 % | längs | ~ 20 ° C |
0,5 - 3 mm | >= 28 % | quer | ~ 20 ° C |
>= 3 mm | >= 30 % | längs | ~ 20 ° C |
>= 3 mm | >= 30 % | quer | ~ 20 ° C |
Langerzeugnisse | ||
geglüht | Bruchdehnung (A5, 65) | bei Temperatur |
<= 25 mm | >= 30 % | ~ 20 ° C |
Walzdraht | ||
lösungsgeglüht | Zugfestigkeit (Rm) | bei Temperatur |
<= 25mm | 450 - 680 N/mm² | ~ 20 ° C |
Profile | ||||
lösungsgeglüht | 0,2% Dehngrenze (Rp0,2) | 1% Dehngrenze (Rp1,0) | Zugfestigkeit (Rm) | Härte [HB] |
<= 25 mm | >= 170 N/mm² | >= 210 N/mm² | 450 - 680 N/mm² | <= 192 HB |