Material 1.4724
Heat-resisting steel
The material 1.4724 is a heat resistant ferritic steel. This material is resistant to scaling up to a maximum temperature of about 850 °C / 1562 °F. 1.4724 is also known under the name Sicromal 9.
Do you have any questions about the material or would you like to order? Complete our inquiry form, it`s free of charge and without obligation. We will get in touch with you in order to provide you with more information.
Standards
HDIN / EN | US-Standard | AFNOR | UNI | JIS | request |
---|---|---|---|---|---|
X10CrAlSi13 X10CrAl13 | request |
Material Category: Heat-resisting steel
Chemical Composition
C % | Si % | Mn % | P % | S % | Al % | Cr % |
max 0,12 | 0,70 - 1,40 | max 1,00 | max 0,040 | max 0,015 | 0,7000 - 1,2000 | 12,00 - 14,00 |
Mechanical Properties
DIN SEW 470 (02/1976) Hitzebeständige Walz- und Schmiedestähle. | |||||
Zeitdehngrenze 1.000 h (Rp 1,0) | Zeitdehngrenze 10.000 h (Rp 1,0) | Zeitstandfestigkeit 1.000 h | Zeitstandfestigkeit 10.000 | Zeitstandfestigkeit 100.000 h | bei Temperatur |
~ 80 N/mm² | ~ 50 N/mm² | ~ 160 N/mm² | ~ 100 N/mm² | ~ 55 N/mm² | ~ 500 ° C |
~ 27,5 N/mm² | ~ 17,5 N/mm² | ~ 55 N/mm² | ~ 35 N/mm² | ~ 20 N/mm² | ~ 600 ° C |
~ 8,5 N/mm² | ~ 4,7 N/mm² | ~ 17 N/mm² | ~ 9,5 N/mm² | ~ 5 N/mm² | ~ 700 ° C |
~ 3,7 N/mm² | ~ 2,1 N/mm² | ~ 7,5 N/mm² | ~ 4,3 N/mm² | ~ 2,3 N/mm² | ~ 800 ° C |
~ 1,8 N/mm² | ~ 1 N/mm² | ~ 3,6 N/mm² | ~ 1,9 N/mm² | ~ 1 N/mm² | ~ 900 ° C |
Flacherzeugnisse | ||||||
geglüht | 0,2% Dehngrenze (Rp0,2) | Zugfestigkeit (Rm) | Bruchdehnung (A5, 65) | Härte [HB] | Probenlage | bei Temperatur |
>= 3 mm | >= 15 % | längs/quer | ~ 20 ° C | |||
5 - 15 mm | >= 13 % | quer | ~ 20 ° C | |||
0,5 - 3 mm | >= 13 % | längs | ~ 20 ° C | |||
<= 12 mm | >= 250 N/mm² | 450 - 650 N/mm² | <= 192 HB | ~ 20 ° C |
Langerzeugnisse | ||
geglüht | Bruchdehnung (A5, 65) | bei Temperatur |
<= 12 mm | >= 15 % | ~ 20 ° C |
Material request