Chemical Composition
C % | Si % | Mn % | P % | S % | Co % | Cr % | Mo % | W % |
0,17 - 0,23 | 0,15 - 0,35 | 0,40 - 0,60 | max 0,035 | max 0,035 | 9,50 - 10,50 | 9,00 - 10,00 | 1,80 - 2,20 | 5,00 - 6,00 |
Mechanical Properties
geglüht | <= 320 HB 30 |
gehärtet | ~ 52 HRC |
angelassen bei ~ 500 ° C | ~ 55 HRC |
angelassen bei ~ 550 ° C | ~ 55 HRC |
angelassen bei ~ 600 ° C | ~ 54 HRC |
angelassen bei ~ 650 ° C | ~ 53 HRC |
angelassen bei ~ 700 ° C | ~ 46 HRC |