Material 1.0503
Heat-treatable steel
C 45 is an unalloyed heat treatable steel. It is mainly being used for general mechanical engineering.
Do you have any questions about the material or would you like to order? Complete our inquiry form, it`s free of charge and without obligation. We will get in touch with you in order to provide you with more information.
Standards
Material Category: Heat-treatable steel
Chemical Composition
C % | Si % | Mn % | P % | S % | Cr % | Cu % | Mo % | N % | Nb % | Ni % |
0,42 - 0,50 | max 0,40 | 0,50 - 0,80 | max 0,045 | max 0,045 | max 0,30 | max 0,20 | max 0,08 | max 0,020 | max 0,030 | max 0,30 |
Mechanical Properties
1.0506 | |||||||
normalgeglüht | Streckgrenze (Re) | Zugfestigkeit (Rm) | Bruchdehnung (A5,65) | bei Temperatur | |||
<= 16 mm | >= 340 N/mm² | >= 620 N/mm² | >= 14 % | ~ 20 ° C | |||
16 - 100 mm | >= 305 N/mm² | >= 580 N/mm² | >= 16 % | ~ 20 ° C | |||
100 - 250 mm | >= 275 N/mm² | >= 560 N/mm² | >= 16 % | ~ 20 ° C |
Weichgeglüht | |
Härte (HBW) | <= 207 HBW |
Vergütet | |||||||||
Abmessung | Streckgrenze (Re) | Zugfestigkeit (Rm) | Bruchdehnung (A5,65) | Einschnürung (Z) | bei Temperatur | ||||
<= 16 mm | >= 340 N/mm² | 700 - 850 N/mm² | >= 14 % | >= 35 % | ~ 20 ° C | ||||
16 - 40 mm | >= 305 N/mm² | 650 - 800 N/mm² | >= 16 % | >= 40 % | ~-20 ° C | ||||
40 - 100 mm | >= 275 N/mm² | 630 - 780 N/mm² | >= 17 % | >= 45 % | ~ 20 ° C | ||||
behandelt auf Scherbarkeit | |
Härte (HBW) | <= 255 HBW |
Flacherzeugnisse | |||||||
normalgeglüht | Streckgrenze (Re) | Zugfestigkeit (Rm) | Bruchdehnung (A5,65) | bei Temperatur | |||
<= 16 mm | >= 340 N/mm² | >= 620 N/mm² | >= 14 % | ~ 20 ° C | |||
16 - 100 mm | >= 305 N/mm² | >= 580 N/mm² | >= 16 % | ~ 20 ° C | |||
100 - 250 mm | >= 275 N/mm² | >= 560 N/mm² | >= 16 % | ~ 20 ° C |
Vergütet | |||||||||
Abmessung | Streckgrenze (Re) | Zugfestigkeit (Rm) | Bruchdehnung (A5,65) | Einschnürung (Z) | bei Temperatur | ||||
<= 8 mm | >= 490 N/mm² | 700 - 850 N/mm² | >= 14 % | >= 35 % | ~ 20 ° C | ||||
8 - 20 mm | >= 430 N/mm² | 650 - 800 N/mm² | >= 16 % | >= 40 % | ~-20 ° C | ||||
20 - 60 mm | >= 370 N/mm² | 630 - 780 N/mm² | >= 17 % | >= 45 % | ~ 20 ° C |