Material 1.0482
Warmfester Baustahl
Do you have any questions about the material or would you like to order? Complete our inquiry form, it`s free of charge and without obligation. We will get in touch with you in order to provide you with more information.
Standards
Material Category: Warmfester Baustahl
Chemical Composition
C % | Si % | Mn % | P % | S % | Cr % |
0,17 - 0,22 C | 0,30 - 0,60 | 1,00 - 1,30 | max 0,040 | max 0,040 | max 0,30 |
Mechanical Properties
Stabstahl | ||||||||||||
vergütet | Streckgrenze (Re) | Zugfestigkeit (Rm) | Bruchdehnung (A5,65) | Härte (HB) | Kerbschlagarbeit KV2 (ISO-V/Charpy-V) | Probenlage | ||||||
<= 60 mm | >= 315 N/mm² | 510 - 610 N/mm² | >= 20 % | 150 - 180 | >= 34 Joule | ~ -20 ° C | längs | |||||
0,2% Dehngrenze (Rp0,2) | Wert | bei Temperatur | ||||||||||
>= 314 N/mm² | ~ 200 ° C | |||||||||||
>= 226 N/mm² | ~ 300 ° C | |||||||||||
>= 206 N/mm² | ~ 350 ° C | |||||||||||
>= 177 N/mm² | ~ 400 ° C | |||||||||||
>= 157 N/mm² | ~ 450 ° C |
DIN EN 10028-2 Flacherzeugnisse aus Druckbehälterstählen. Unlegierte und legierte Stähle mit festgelegten Eigenschaften bei erhöhten Temperaturen. | ||||||||||
Zeitdehngrenze 1.000 h (Rp 1,0) | Zeitdehngrenze 10.000 h (Rp 1,0) | Zeitdehngrenze 100.000 h (Rp 1,0) | Zeitstandfestigkeit 10.000 h | Zeitstandfestigkeit 100.000 h | ||||||
Wert | bei Temperatur | Wert | bei Temperatur | Wert | bei Temperatur | Wert | bei Temperatur | Wert | bei Temperatur | |
~ 147 N/mm² | ~ 450 °C | ~ 108 N/mm² | ~ 450 °C | ~ 64 N/mm² | ~ 450 °C | ~ 137 N/mm² | ~ 450 °C | ~ 83 N/mm² | ~ 450 °C | |
~ 83 N/mm² | ~ 500 °C | ~ 55 N/mm² | ~ 500 °C | ~ 31 N/mm² | ~ 500 °C | ~ 76 N/mm² | ~ 500 °C | ~ 44 N/mm² | ~ 500 °C |