Material 1.0460
High-temperature constructional steel
C22.8 / ASTM A 105 is an unalloyed quality steel. This steel grade is available from stock either as hot-rolled or forged bars. C22.8 / ASTM A 105 is normalized as well as extensively affirmed as well as C22.8 is available from stock with certificate 3.1 according AD 2000 W13. Mainly it is being used to produce fittings, ball valves or flanges.
Do you have any questions about the material or would you like to order? Complete our inquiry form, it`s free of charge and without obligation. We will get in touch with you in order to provide you with more information.
Standards
Material Category: High-temperature constructional steel
Chemical Composition
C % | Si % | Mn % | P % | S % | Al % | Cr % | Cu % | Mo % | N % | Nb % | Ni % | Ti % | V % |
0,18 - 0,23 | max 0,40 | 0,30 - 0,90 | max 0,025 | max 0,015 | min 0,0200 | max 0,30 | max 0,30 | max 0,08 | max 0,012 | max 0,020 | max 0,30 | max 0,03 | max 0,02 |
Mechanical Properties
DIN EN 10273 Warmgewalzte schweißgeeignete Stäbe aus Stahl für Druckbehälter mit festgelegten Eigenschaften bei erhöhten Temperaturen. | |||||||
normalgeglüht | Streckgrenze (Re) | Zugfestigkeit (Rm) | Bruchdehnung (A5,65) | ||||
<= 50 mm | >= 250 N/mm² | 410 - 540 N/mm² | >= 25 % | ||||
50 - 100 mm | >= 240 N/mm² | 410 - 540 N/mm² | >= 25 % | ||||
100 - 150 mm | >= 230 N/mm² | 410 - 540 N/mm² | >= 25 % | ||||
Stäbe Kerbschlagarbeit KV2 (ISO-V/Charpy-V) | |||||||
Wert | Probenlage | bei Temperatur | |||||
>= 27 J | längs | ~ -20 ° C | |||||
>= 40 J | längs | ~ 0 ° C | |||||
>= 47 J | längs | ~ 20 ° C | |||||
0,2% Dehngrenze (Rp0,2) | Wert | bei Temperatur | |||||
<= 50 mm | >= 240 N/mm² | ~ 20 ° C | |||||
<= 50 mm | >= 242 N/mm² | ~ 50 ° C | |||||
<= 50 mm | >= 237 N/mm² | ~ 100 ° C | |||||
<= 50 mm | >= 216 N/mm² | ~ 150 ° C | |||||
<= 50 mm | >= 190 N/mm² | ~ 200 ° C | |||||
<= 50 mm | >= 170 N/mm² | ~ 250 ° C | |||||
<= 50 mm | >= 150 N/mm² | ~ 300 ° C | |||||
<= 50 mm | >= 130 N/mm² | ~ 350 ° C | |||||
<= 50 mm | >= 110 N/mm² | ~ 400 ° C | |||||
<= 50 mm | >= 90 N/mm² | ~ 450 ° C | |||||
50 - 100 mm | >= 230 N/mm² | ~ 20 ° C | |||||
50 - 100 mm | >= 234 N/mm² | ~ 50 ° C | |||||
50 - 100 mm | >= 230 N/mm² | ~ 100 ° C | |||||
50 - 100 mm | >= 210 N/mm² | ~ 150 ° C | |||||
50 - 100 mm | >= 185 N/mm² | ~ 200 ° C | |||||
50 - 100 mm | >= 165 N/mm² | ~ 250 ° C | |||||
50 - 100 mm | >= 145 N/mm² | ~ 300 ° C | |||||
50 - 100 mm | >= 125 N/mm² | ~ 350 ° C | |||||
50 - 100 mm | >= 100 N/mm² | ~ 400 ° C | |||||
50 - 100 mm | >= 80 N/mm² | ~ 450 ° C | |||||
100 - 150 mm | >= 220N/mm² | ~ 20 ° C | |||||
100 - 150 mm | >= 224 N/mm² | ~ 50 ° C | |||||
100 - 150 mm | >= 220 N/mm² | ~ 100 ° C | |||||
100 - 150 mm | >= 200 N/mm² | ~ 150 ° C | |||||
100 - 150 mm | >= 175 N/mm² | ~ 200 ° C | |||||
100 - 150 mm | >= 155 N/mm² | ~ 250 ° C | |||||
100 - 150 mm | >= 135 N/mm² | ~ 300 ° C | |||||
100 - 150 mm | >= 115 N/mm² | ~ 350 ° C | |||||
100 - 150 mm | >= 90 N/mm² | ~ 400 ° C | |||||
100 - 150 mm | >= 70 N/mm² | ~ 450 ° C |